Refining Agents and Fluxes for Aluminum Melt


Article Translation

1. What Refining Agent Is Suitable for the First Refini ng Process?

During first refining, solid refining agents or a chlorine-nitrogen mixed gas can be used as the refining agent. These are traditional refining agents commonly used in aluminum alloy production.

Chlorine and chlorine gas, especially chlorine, are very effective in removing non-metallic inclusions from aluminum melt. However, chlorine is toxic and causes serious environmental pollution, so its use must be strictly limited. One purpose of using a chlorine-nitrogen mixed gas is to greatly reduce chlorine consumption.

In recent years, nitrogen-sprayed powdered flux has been used to refine aluminum melt. This method combines the advantages of solid flux refining and chlorine-nitrogen mixed gas refining, and it is worth wider application.

2. What Is Flux?

Flux refers to salt-based refining materials used during aluminum and aluminum alloy melting. Most fluxes are solid compound salts. Fluxes used for aluminum melt refining are generally composed of alkali metal or alkaline earth metal halide salts.

According to their functions, fluxes can be divided into covering fluxes, degassing agents, refining agents, drossing agents, furnace-cleaning agents, magnesium-removal agents, sodium-removal agents, and calcium-removal agents.

The composition of a flux depends on its intended use. A covering flux generally requires low surface tension and a low melting point. A drossing flux should have relatively high surface tension against the aluminum melt and relatively low surface tension against oxide dross. To improve dross removal efficiency, it is also desirable for the flux to generate heat. A refining flux should have good adsorption capacity and a certain dissolving ability for aluminum oxide. It should also generate an appropriate amount of gas to achieve good degassing results.

Common Compound Fluxes for Wrought Aluminum and Aluminum Alloys

Flux No.Main Composition / Mass Fraction
No. 1KCl 47%, NaCl 30%, Na3AlF6 23%
No. 2KCl 40%, MgCl2 46%, CaCl2 <=8%, BaCl2 8%
No. 3KCl 50%, NaCl 50%
No. 4CaF2 40%, MgCl2-KCl 60%
No. 5CaF2 20%, MgCl2-KCl 80%
No. 6Na3AlF6 50%, C2Cl6 50%
No. 7KCl 11.5%, NaCl 56.5%, Na3AlF6 7%, NaF 25%
No. 8KCl 10%, NaCl 50%, Na3AlF6 10%, NaF 30%
No. 9NaCl 45%, Na3AlF6 15%, NaF 40%
No. 10NaCl 25%, Na3AlF6 15%, NaF 60%
No. 11KCl 12.5%, NaCl 62.5%, Na3SiF6 25%
No. 12KCl 45%, LiCl 55%
No. 13KCl 18%, LiCl 25-35%, AlF3 4-10%, MgCl2-KCl 30-50%
No. 14KCl 40-50%, LiCl 40-50%, AlF3 4-10%
No. 15LiCl 45-50%, MgCl2-KCl 45-55%

Notes: No. 1 and No. 6 fluxes are used for Series 1, 2, 3, and 7 aluminum alloys. No. 2 flux is used for high-magnesium alloys. No. 3 flux is used as a covering flux for scrap remelting. No. 4 and No. 5 fluxes are used for low-magnesium and Series 6 aluminum alloys. No. 7 to No. 11 fluxes are used for Series 4 aluminum alloys. No. 12 to No. 15 fluxes are respectively used for covering lithium-containing aluminum alloys, electrolytic flux refining, and crystallizer protection.

Factors Affecting Crucible Service Life

In high-temperature sintering, the sintered structure changes as smelting heats increase. After use, the sintered layer of the crucible accounts for about 40%-50% of the wall thickness, while the semi-sintered layer accounts for about 30%-35%.

5. Influence of the Smelting Process

1. Influence of Smelting Temperature

If the molten steel temperature is too high, the slag temperature will also rise, which accelerates crucible erosion and causes premature damage along the slag line. Overheated molten steel has better fluidity and can penetrate cracks more quickly, leading to rapid crucible failure.

In addition, high-temperature molten steel promotes reactions between the molten steel and crucible material, accelerating chemical erosion of the crucible. In short, the higher the smelting temperature, the shorter the crucible service life.

2. Influence of Steel Grade

When smelting steels with low melting points and good fluidity, such as high-carbon and high-manganese steels, the molten steel penetrates the crucible more strongly, reducing its service life.

When smelting steel grades with poor fluidity, such as low-carbon and high-nickel-chromium steels, the crucible usually has a longer service life. Therefore, when planning steel production, high-carbon and high-manganese steels should be arranged in the later stage of crucible use.

3. Influence of Slag Properties

The basicity of furnace slag should match the crucible material. Magnesia crucibles are severely corroded by slag with high CaO and SiO2 content. The CaF2 content in the slag should also be controlled, because excessive CaF2 will corrode the basic furnace lining and cause premature melting of the slag-line area.

Basic slag is suitable for magnesia crucibles, while acidic slag is suitable for silica crucibles. Alumina-magnesia crucibles should only use weakly basic or neutral slag. The slag should be selected according to the crucible material.

When smelting is carried out under vacuum without slag, the crucible service life is longer than in non-vacuum smelting. This shows that furnace slag reduces crucible service life.

4. Influence of Smelting Operation

During the melting stage, the formation of “bridging” in the charge has a major impact on crucible service life. When bridging occurs, the charge separates from the molten steel, and the molten steel temperature can become excessively high. This seriously affects crucible life. Strong vibration or hammering used to eliminate bridging may also damage the crucible.

Crucible Maintenance

Correct use and maintenance are important ways to extend crucible service life. In addition to controlling the factors mentioned above, maintenance should be strengthened in the following areas.

1. Use and Maintenance of New Crucibles

New crucibles should be carefully maintained during early use, especially low-temperature sintered crucibles. Potential defects in a new crucible often appear during the first few smelting heats, and steel leakage accidents usually occur in the first several heats.

Therefore, every step from charging and melting to controlling the smelting temperature must be handled carefully to ensure smooth operation. In the early stage, avoid smelting high-carbon and high-manganese steels with good fluidity as much as possible. Low-carbon and low-alloy steels are more suitable. The slag should have a relatively high viscosity. After tapping, carefully inspect the inner wall of the crucible for obvious cracks.

During smelting with a new crucible, pay attention to changes in electrical parameters. Under normal conditions, voltage and current remain stable. If the crucible becomes abnormal, the voltage and current will change, usually showing a drop in voltage and a rise in current. If abnormal electrical parameters appear, the furnace should be stopped immediately for inspection and treatment to prevent steel leakage.

2. Reasonable Arrangement of Smelting Heats

For intermittent operation, production should be concentrated as much as possible to reduce the number of furnace shutdowns and help extend crucible service life.

During the full service cycle of a crucible, the steel grades should be arranged properly. In the early stage, low-carbon and low-alloy steels should be smelted first. In the middle stage, high-alloy steels can be arranged. In the later stage, high-carbon steel grades are more suitable.

When smelting cast iron in a medium-frequency induction furnace, if smelting is interrupted for a short period, heat preservation measures can be taken. For example, the crucible can be electrically heated to keep the temperature at 600-800°C, or a certain amount of molten iron can be retained for holding. This helps improve crucible service life.

3. Timely Repair and Cleaning of the Crucible Inner Wall

Steel leakage from a crucible is mostly caused by cracks and local erosion. After tapping, use special slag-removal tools immediately to remove residual slag adhering to the inner wall, and check for cracks or local erosion.

If cracks or local erosion are found, repair them promptly. After the crucible cools, remove exposed sintered layers from the slag area. Then use a mixture of fine-powder sand material, brine, and water glass to repair the damaged area, followed by drying.


We use optional cookies to improve your experience on our site, including through social media connections, and to serve personalized ads based on your online activity. If you refuse optional cookies, we will only use cookies that are necessary to provide you with the service.  Privacy Statement

Leave your inquiry now, and get a systematic solution later.

We will contact you within one working day. Please pay attention to your email.

Submit message